⚡Parameter Wizard

Enter the job — get tiered starting points with the reasoning behind them.

Conservative

Amperage163 A
Voltage18.7 V
Wire feed326 ipm
Travel speed4.9 ipm
Heat input30 kJ/in

Recommended

Start here
Amperage185 A
Voltage19.4 V
Wire feed370 ipm
Travel speed5.7 ipm
Heat input30 kJ/in

Aggressive

Amperage213 A
Voltage20.3 V
Wire feed426 ipm
Travel speed6.9 ipm
Heat input30 kJ/in

Setup

Polarity
DCEP
Gas flow
30 CFH
CTWD / stickout
0.375 in
Work angle
45°
Travel angle
10°
Direction
push
Filler dia
.035"
Pass sequence

Root + 1–2 cover passes; weave or split layers for larger leg sizes.

Transfer mode

Short-circuit: wire dips into the puddle and shorts ~20–200×/sec. Low heat — best for thin material and out-of-position, but watch for cold lap / lack of fusion on thick steel.

Why these settings

  • Short-circuit MIG on Carbon Steel (A36 / mild) at 0.25" — centered ~185 A on 0.035" electrode, DCEP.
  • WFS derived from amperage via 0.035" burn-off rate; voltage set for short transfer.
  • Travel speed solved to hit a moderate heat-input band for this thickness/metal; three tiers bracket it.
⚠ Starting point, not code approval. These are practical starting points from a rules engine — fine-tune on a test coupon and verify any code work (AWS/ASME/API) with your qualified welding engineer or CWI.